Round robin prueba el análisis XRF XRF EQAS St Gobain - SGIB, vidrio borosilicato
VAT No.:
San Gobain Isover - CRIR
Material de comparación entre laboratorios:
SGIB, vidrio borosilicato
Estudio terminado:
2002 - 6
Bibliografía:
Informe final
elementos principales [wt %]
CRB | RV | 1sRV | Z-Score | |
Na₂O | 15,780 | 15,810 | 0,130 | --- |
MgO | 3,080 | 3,200 | 0,100 | --- |
Al₂O₃ | 1,610 | 1,600 | 0,070 | --- |
SiO₂ | 65,440 | 65,780 | 0,320 | --- |
P₂O5 | 0,030 | 0,030 | 0,007 | --- |
SO₃ | 0,090 | 0,080 | 0,030 | --- |
K₂O | 0,600 | 0,610 | 0,030 | --- |
CaO | 7,660 | 7,600 | 0,150 | --- |
TiO₂ | 0,028 | 0,030 | 0,007 | --- |
Fe₂O₃ tot. | 0,210 | 0,240 | 0,020 | --- |
MnO | 0,407 | 0,410 | 0,023 | --- |
oligoelementos [µg/g]
CRB | RV | 1sRV | Z-Score | |
Ba | 200,00 | --- | --- | --- |
Cr | 90,00 | --- | --- | --- |
Rb | 10,00 | --- | --- | --- |
Sr | 10,00 | --- | --- | --- |
Zr | 320,00 | --- | --- | --- |
Leyenda
CRB
resultados CRB
essai interlaboratorios
Resultados del estudio colaborativo
1s-RV
Estudio colaborativo de desviación estándar
Z-Score
Diferencia entre el valor medido y el estudio promedio
*
Valor no certificado