Round robin prueba el análisis XRF Prueba XRF EQAS GSJ - JCFA-1, Ceniza de mosca de carbón
VAT No.:
Servicio Geológico de Japón (GSJ)
Material de comparación entre laboratorios:
JCFA-1, Ceniza de mosca de carbón
Estudio terminado:
2003 - 1
Bibliografía:
en la web en http://www.iaea.or.at
elementos principales [wt %]
CRB | RV | 1sRV | Z-Score | |
Na₂O | 2,220 | 2,240 | --- | --- |
MgO | 2,270 | 2,300 | --- | --- |
Al₂O₃ | 24,290 | 24,250 | --- | --- |
SiO₂ | 50,470 | 50,560 | --- | --- |
P₂O5 | 0,573 | 0,586 | --- | --- |
SO₃ | 0,480 | 0,490 | --- | --- |
K₂O | 1,190 | 1,270 | --- | --- |
CaO | 8,730 | 8,910 | --- | --- |
TiO₂ | 1,340 | 1,310 | --- | --- |
Fe₂O₃ tot | 5,140 | 5,200 | --- | --- |
MnO | 0,063 | 0,068 | --- | --- |
C total | 1,460 | 1,350 | --- | --- |
oligoelementos [µg/g]
CRB | RV | 1sRV | Z-Score | |
As | 25,00 | 29,10 | --- | --- |
Co | 37,00 | 37,40 | --- | --- |
Cr | 89,00 | 75,00 | --- | --- |
Cu | 126,00 | 129,00 | --- | --- |
Ni | 32,00 | 21,00 | --- | --- |
Pb | 56,00 | 47,20 | --- | --- |
Rb | 52,00 | 54,10 | --- | --- |
Sr | 1078,00 | 110,00 | --- | --- |
V | 238,00 | 243,00 | --- | --- |
Zn | 65,00 | 6,00 | --- | --- |
Leyenda
CRB
resultados CRB
essai interlaboratorios
Resultados del estudio colaborativo
1s-RV
Estudio colaborativo de desviación estándar
Z-Score
Diferencia entre el valor medido y el estudio promedio
*
Valor no certificado