Round robin tests XRF-analysis XRF Round-robin test NRCGA-CAGS, China - Marines Sediment GSMS-5
Study organized by:
National Research Center for Geoanalysis - Chinese Academy of Geological Sciences
Material of proficiency test:
GBW 07335 (GSMS-5, Marines Sediment)
Study finished:
2010 - 11
Literature:
Zertifikat Ringversuchsveranstalter
major elements [wt %]
CRB | RV | 1sRV | Z-Score | |
Na₂O | 2,100 | 2,300 | 0,200 | |
MgO | 2,500 | 2,510 | 0,090 | |
Al₂O₃ | 13,320 | 13,100 | 0,200 | |
SiO₂ | 59,400 | 59,600 | 0,200 | |
P₂O5 | 0,122 | 0,120 | 0,010 | |
SO₃ | 0,250 | 0,220 | 0,010 | |
K₂O | 2,700 | 2,710 | 0,060 | |
CaO | 4,780 | 4,800 | 0,200 | |
TiO₂ | 0,700 | 0,720 | 0,030 | |
Fe₂O₃ tot | 5,270 | 5,200 | 0,200 | |
MnO | 0,077 | 0,073 | 0,005 | |
L.O.I.* | 8,540 |
trace elements [µg/g]
CRB | RV | 1sRV | Z-Score | |
As | 13,00 | 8,00 | ||
Ba | 407,00 | 396,00 | 19,00 | |
Cd | 0,40 | 0,20 | ||
Ce | 97,00 | 78,00 | 4,00 | |
Cl [%] | 1,05 | 1,04 | 0,06 | |
Co | 16,00 | 15,00 | 1,00 | |
Cr | 83,00 | 78,00 | 10,00 | |
Cu | 18,00 | 18,00 | 4,00 | |
F [%] | 0,087 | |||
Ga | 17,00 | 16,00 | 2,00 | |
Hf | 5,00 | 5,00 | 0,40 | |
La | 23,00 | 38,00 | 2,00 | |
Nb | 10,00 | 13,70 | 0,80 | |
Nd | 25,00 | 32,60 | 2,30 | |
Ni | 31,00 | 36,00 | 5,00 | |
Pb | 30,00 | 25,00 | 4,00 | |
Pr | 5,00 | 8,30 | 0,30 | |
Rb | 118,00 | 118,00 | 3,00 | |
Sm | 5,00 | 6,20 | 0,30 | |
Sr | 204,00 | 193,00 | 8,00 | |
Th | 13,00 | 13,60 | 0,60 | |
U | 1,80 | 2,70 | 0,40 | |
V | 90,00 | 95,00 | 9,00 | |
Y | 24,00 | 25,00 | 2,00 | |
Zn | 85,00 | 79,00 | 8,00 | |
Zr | 181,00 | 184,00 | 24,00 |
Legend
CRB
results CRB
cooperative test
results collaborative study
1s-RV
Standard deviation collaborative study
Z-Score
Difference of measured value from mean study
*
Value not certified